1, Standard proportation: main adhesive: firming agent=10:2. When the air moisture is more than 80%, the firming agent should be added properly during polyurethane ink brush mark.
2, Dilution: adding ethyl acetate in main adhesive.
3, The change of work concentration and viscosity diluted by ethyl acetate is shown as the picture.
PU-170-1A(kg) |
PU-170-1B(kg) |
Ethyl acetate(kg) |
Work concentration(%) |
Viscosity (s) |
10 |
2 |
10.9 |
35 |
21-23 |
10 |
2 |
13.0 |
32 |
18-20 |
10 |
2 |
14.7 |
30 |
16-18 |
10 |
2 |
16.6 |
28 |
14-16 |
10 |
2 |
20.0 |
25 |
13-15 |
4, Glue spread calculation formula: dry glue spread (g/m2 ) =1/5~1/6×work concentration%×net depth, including 1/5~1/6 percent conversion.
5, Complex high stewing antiseptic package bag, dry glue spread should not be lower than 4g/m2 , the recommended work concentration 32%.
6, In order to promote solvent volatilization in foil glue, try to increase dry efficiency of compounding machine.
7, Lamination:Try to increase complex hot quinine temperature and pressure and the hot quinine temperature can be chosen between 50~90℃.
8, Curing:After composition, it should be sent to curing room as soon as possible. Under the 50±5℃ condition, curing for 36-48 hours can achieve prospective strength. |